Skip to Content
MilliporeSigma
HomeBiopharmaceutical CharacterizationBiosimilar Comparability Workflow for Intact Mass Analysis

Biosimilar Comparability Workflow for Intact Mass Analysis Using Trastuzumab as Model Protein

Geoffrey Rule1, Sundaram Palaniswamy2, Uma Sreenivasan3, Paresh Tank4, Fatima D’Souza4

1Bellefonte, PA, USA, 2Bangalore, India, 3Round Rock, TX, USA, 4ZRAS, Zelle Biotechnology Pvt. Ltd., Thane, India

Introduction

Biosimilar mAb drugs have surged in the last decade due to patent expiration of innovator drugs, offering affordable care to patients. Biosimilars, while sharing amino acid sequences with innovators, can differ structurally due to post-translational modifications (PTMs) resulting from changes in manufacturing processes. These variations, like N-glycosylation and alterations to termini, pose challenges in proving comparability.1

Thorough characterization of therapeutic mAbs is vital for safety and efficacy and establishing critical quality attributes (CQAs) are essential for both innovator and biosimilar drugs.2,3 Characterization generally involves chromatography (e.g., SEC, RP, HILIC) combined with mass spectrometry (MS).

Trastuzumab received approval for medical usage in the United States in September 1998 and in the European Union in August 2000. At present, five biosimilars have gained approval in both the European Union and the United States.4,5

This application describes the utilization of a nonreducing RPLC-MS workflow for intact mass comparison of trastuzumab innovator and biosimilar. The report includes the correlation of de-charged, observed masses with theoretical masses.

A recombinant human antibody standard, SILu™Lite SigmaMAb™  (MSQC4), is utilized as a reference and assay control sample. Here, this is referred to simply as SigmaMAb™  although several other SigmaMAb™ standards are also available commercially.


Workflow for Intact Mass Analysis of Trastuzumab

Antibody reduction (optional)

Icon for optional reduction process

    Chromatography

    Icon for chromatography

      Measurement and Analysis

      Icon for measurement and analysis

        A complete RPLC-MS workflow has been developed to simplify intact mass analysis of non-reduced monoclonal antibodies (mAbs) for biosimilarity assessment.

        In detail, it includes:

        • Mass spectrometer calibration
        • System suitability test utilizing a recombinant human monoclonal antibody reference
        • A generic RPLC-MS method compatible with sample separation and analysis of both non-reduced and reduced monoclonal antibodies

        Experimental - Sample and Reference Preparation and System Setup

        Instrument Calibration

        The Waters QToF Xevo G2XS mass spectrometer was calibrated in a mass range of 400 – 4000 m/z with a 10 μL/min infusion of 0.4 mg/mL of sodium iodide in water. Alternatively, calibration can be performed with a 10 μL/min infusion of 0.4 mg/mL cesium iodide, polyalanine in water prior to running the samples.

        System Suitability

        To evaluate performance of the entire workflow, an assay control (SigmaMAb™) was prepared and analyzed along with the samples. SigmaMAb™ reference was tested to ensure system suitability.

        RPLC-MS System Setup and MS Data Analysis

        RPLC-MS System Setup

        The essential settings of the UHPLC-PDA chromatography system and the qToF mass spectrometer applied in the analysis of non-reduced antibodies are listed in Tables 1 and 2 below.

        LC  Conditions

        Instrument:

        Waters™ H-Class Acquity UPLC Chromatography System

        Software:

        UNIFI

        Column:

        BIOshell™ A400 Protein C4, 100 x 2.1 mm I.D., 3.4 μm (66825-U)

        Mobile phase:

        [A] Water + 0.1% FA; [B] acetonitrile + 0.1% FA

        Gradient:

        See Table 1b

        Flow:

        0.2 mL/min

        Column temp:

        80 °C

        Autosampler temp:

        8 °C

        Run time:

        10 min

        Detector:

        PDA 280 nm and MS TOF (see Table 2 for conditions)

        Flow divert:

        1.0 –10.0 min

        Loop volume:

        10 μL

        Injection method:

        Partial loop or full loop

        Injection volume:

        1 μL for intact mass

        Table 1.UHPLC-PDA settings.

        Time (min)

        %A

        %B

        Curve

        0.00

        95.0

        5.0

        Initial

        1.00

        95.0

        5.0

        6

        3.50

        40.0

        60.0

        6

        5.00

        40.0

        60.0

        6

        5.50

        5.0

        95.0

        6

        7.50

        5.0

        95.0

        6

        7.60

        95.0

        5.0

        6

        10.00

        95.0

        5.0

        6

        Table 1b.Gradient Table for intact mass analysis

        MS Conditions

         

        Instrument:

        Waters™ QToF Xevo G2X2 Mass Spectrometer

        Software:

        UNIFI

        Capillary (V):

        3,000

        Sample cone (V)

        40

        Extraction cone (V):

        3

        Ion guide (V):

        3

        Desolvation temp (° C):

        100

        Source temp (° C):

        120

        Scan range (Da):

        400 – 4,000

        Desolvation gas (L/h):

        800

        Cone gas (L/h):

        50

        Collision energy (V):

        5

        Pusher (V):

        930

        RF Setting:

        Autoprofile

        Table 2.qToF-MS settings

        MS Data Analysis

        Data were processed using the MaxEnt1 module within the UNIFI software to generate and analyze deconvoluted (zero charged) mass spectra. In general, a summed spectrum was created from the corresponding total ion chromatogram (TIC) of the eluted intact mAb. The summed m/z spectrum was then processed by the MaxEnt1 algorithm; detailed parameters are listed in Table 3.

        For glycoform analysis, data were processed using UNIFI software from Waters™. Glycoforms were matched by the software. Glycoform relative abundance data were tabulated based on peak intensities of the coeluting glycoform species.

        Non-Reduced Intact Mass

        m/z Range:

        2,000 – 3,500

        Mass range (Da):

        140,000 - 160,000

        Output resolution:

        1 Da

        Peak width model:

        tof

        TOF resolution:

        10,000

        Minimum intensity ratios, L and R (%):

        30

        Iterations:

        12

        Table 3.Deconvolution parameters.

        Results

        The analysis objective here, was to perform non-reduced RPLC-MS intact mass analysis on all submitted samples to compare the molecular weight of trastuzumab innovator and biosimilar drugs.

        Intact SigmaMAb™ was used to determine system suitability. All mAb samples were solubilized in 100 μL water to a final concentration of 1 mg/mL.

        System Suitability Test Results

        SigmaMAb reference sample (1 μL) was injected on the RPLC-MS system. Figure 1 illustrates the photodiode array (280 nm) and TIC (total ion current) traces of the non-reduced antibody, while Figure 2 displays the deconvoluted mass spectrum of the SigmaMAb™ reference. The observed intact mAb glycoforms matched the common glycoform masses of MSQC4, as listed in Table 4. The measured discrepancies between the observed masses and the theoretical values for four glycoforms are all within 0.011 % mass error.

        A UV chromatogram of non-reduced SigmaMAb reference standard, measured at 280 nm, displays a distinct peak at 4.72 minutes, with absorbance on the y-axis and retention time on the x-axis.
        A TIC chromatogram of non-reduced SigmaMAb reference standard displays a distinct peak at 4.84 minute, with total ion current on the y-axis and retention time on the x-axis.

        Figure 1. Photodiode array (280 nm, left) and TIC traces (right) of non-reduced SigmaMAb™ reference.

        Summed mass spectra for non-reduced SigmaMAb reference with intensity measured in counts on the y-axis and observed mass on the x-axis
        Deconvoluted mass spectra obtained for non-reduced SigmaMAb reference (MSQC4) with six distinct peaks at observed mass values of 146524, 146674, 146831, 146990, 147157, and 147311.

        Figure 2. MS data for non-reduced SigmaMAb™ reference (MSQC4). Left: summed spectrum; right: deconvoluted spectrum.

        Species

        Molecular Formula

        Theoretical Mass (Da)*

        Observed Mass (Da)

        Error (Da)

        Error (%)

        Heavy Chain/G0FG0F

        C6486H10048N1716O2070S46

        146658

        146675

        17

        +0.011

        Heavy Chain/G0FG1F

        C6492H10058N1716O2075S46

        146821

        146833

        12

        +0.008

        Heavy Chain/G1FG1F

        C6498H10068N1716O2080S46

        146983

        146994

        11

        +0.007

        Heavy Chain/G1FG2F

        C6504H10078N1716O2085S46

        147145

        147156

        11

        +0.007

        Heavy Chain/G2FG2F

        C6510H10088N1716O2090S46

        147307

        147310

        3

        +0.002

        G0F: GlcNAc2Man3GlcNAc2Fuc

        G1F: GalGlcNAc2Man3GlcNAc2Fuc

        G2F: Gal2GlcNAc2Man3GlcNAc2Fuc

        *Masses based on NIST Physical Reference Data

        Table 4.Observed and theoretical masses of non-reduced SigmaMAb™ reference glycoforms

        Non-Reduced Sample Results

        The monoclonal antibody samples were analyzed in their non-reduced form using RPLC-MS. The corresponding photodiode array (280 nm) traces, TICs, MS spectra and the deconvoluted MS spectra of trastuzumab innovator and biosimilar are shown in Figures 3 and 4. The relative quantitation results for N-glycoform distribution are shown in Figure 5. The method detects differences in the distribution of major N-glycoforms between innovator and biosimilar products. The observed masses of the non-reduced mAb correlate well with the calculated theoretical masses for all submitted samples, as shown in Table 5, and the observed mass error is 0.004% or less.

        A UV chromatogram of non-reduced trastuzumab, measured at 280 nm, exhibits a distinct peak at 4.67 minutes. The innovator is represented by a red curve, while the biosimilar is depicted by a blue curve, with absorbance on the y-axis and retention time on the x-axis.
        A TIC chromatogram of fully reduced trastuzumab, exhibits a distinct peak at 4.79 minutes. The innovator is represented by a red curve, while the biosimilar is depicted by a blue curve, with absorbance on the y-axis and retention time on the x-axis.

        Figure 3. Comparative photodiode array (280 nm, left) and TIC traces (right) of non-reduced trastuzumab. Red: Innovator; blue: Biosimilar.

        Summed up mass spectra for non-reduced trastuzumab. The innovator is represented by a red curve, while the biosimilar is depicted by a blue curve, with intensity measured in counts on the y-axis and observed mass on the x-axis.
        The deconvoluted mass spectra for non-reduced trastuzumab reveals distinct peaks at mass values of 148059, 148221, 148383, and 148546 from left to right. The innovator is depicted by a red curve, and the biosimilar by a blue curve, with intensity measured in counts on the y-axis and observed mass on the x-axis.

        Figure 4. Comparative MS data for non-reduced trastuzumab. Left: summed spectrum; right: deconvoluted spectrum. Red: Innovator; blue: Biosimilar

        A bar graph depicting the distribution of major N-glycoforms of trastuzumab by Intact RPLC-MS. The innovator is depicted in red curve, and the biosimilar in blue, with relative abundance measured on the y-axis.

        Figure 5.N-glycoform distribution of trastuzumab by Intact RPLC-MS. Red: Innovator; Blue: Biosimilar.

        Species

        Theoretical Mass

        (Da)*

        Observed Mass (Da)

        Error (Da)

        Error (%)

        Innovator

        Biosimilar

        Innovator

        Biosimilar

        Innovator

        Biosimilar

        Heavy Chain/G0FG0F

        148056

        148061

        148061

        +5

        +5

        +0.003

        +0.003

        Heavy Chain/G0FG1F

        148218

        148222

        148223

        +4

        +5

        +0.003

        +0.003

        Heavy Chain/G1FG1F

        148380

        148384

        148386

        +4

        +6

        +0.003

        +0.004

        Heavy Chain/G1FG2F

        148542

        148546

        148547

        +4

        +5

        +0.003

        +0.003

        Heavy Chain/G2FG2F

        148704

        148707

        148705

        +3

        +1

        +0.002

        +0.001

        G0F: GlcNAc2Man3GlcNAc2Fuc

        G1F: GalGlcNAc2Man3GlcNAc2Fuc

        G2F: Gal2GlcNAc2Man3GlcNAc2Fuc

        *Masses based on NIST Physical Reference Data

        Table 5.Calculated and experimental masses of non-reduced trastuzumab

        Conclusion

        Ensuring the regulatory approval of biosimilar monoclonal antibody (mAb) drug products necessitates a meticulous and effective comparability assessment to guarantee their safety and efficacy. This application note serves as an illustration of the utilization of reversed-phase liquid chromatography-mass spectrometry (RPLC-MS) at the intact level. The primary objective revolves around assessing the comparability between the original trastuzumab drug and its biosimilar counterpart. A comprehensive workflow was devised for intact mass analysis of non-reduced monoclonal antibodies, using trastuzumab as a representative mAb, and a SILu™Lite SigmaMAb™ product, as an assay control.

        A separate workflow (Application Note: Biosimilar Comparability Workflow by Middle-Up Mass Analysis Using Trastuzumab as Model Protein - Protocol for reduction and RPLC-MS analysis of a monoclonal antibody) describes an optional mAb reduction procedure which can be performed with either a partial, or full, reduction procedure. Depending on the procedure used, intra-chain disulfide bonds remain intact (partial reduction) or are broken (full reduction). Solutions of sodium iodide, or cesium iodide, were used for mass spectrometer calibration, and a system suitability test, utilizing a recombinant human monoclonal antibody reference, were developed for routine use. In addition, an RP method suitable for separation and analysis of both reduced and non-reduced mAbs was established using a wide-pore, superficially porous C4 column.

        Results obtained from the non-reduced SigmaMAb™ reference indicated minimal disparities of 0.011% mass error, or less, between observed and theoretical masses for four glycoforms. For trastuzumab, both the innovator and biosimilar samples displayed a strong concurrence between observed and theoretical non-reduced mAb masses, with an observed mass error of 0.004%, or lower.

        The experimental findings affirm the versatility of the workflow for analyzing non-reduced monoclonal antibody samples, delivering accurate results that enable distinct identification of multiple glycoforms.

        See more applications on the Biopharmaceutical Characterization page.

        References

        1.
        Review and Approval. 2022 Dec 13 . [Internet]. U.S. Food and Drug Administration. Available from: https://www.fda.gov/drugs/biosimilars/review-and-approval
        2.
        Sandra K, Vandenheede I, Sandra P. 2014. Modern chromatographic and mass spectrometric techniques for protein biopharmaceutical characterization. Journal of Chromatography A. 133581-103. https://doi.org/10.1016/j.chroma.2013.11.057
        3.
        Berkowitz SA, Engen JR, Mazzeo JR, Jones GB. 2012. Analytical tools for characterizing biopharmaceuticals and the implications for biosimilars. Nat Rev Drug Discov. 11(7):527-540. https://doi.org/10.1038/nrd3746
        4.
        Biosimilars approved in the US. Gabionline.net. [Internet]. Available from: https://www.gabionline.net/biosimilars/general/biosimilars-approved-in-the-us
        5.
        Biosimilars approved in Europe. Gabionline.net. [Internet]. Available from: https://www.gabionline.net/biosimilars/general/biosimilars-approved-in-europe
        6.
        Protocol for purification, optional reduction, and SEC-MS analysis of a monoclonal antibody. [Internet]. Sigmaaldrich.com. Available from: /CA/en/technical-documents/protocol/pharmaceutical-and-biopharmaceutical-manufacturing/biologics-biosimilars-characterization/protocol-for-analysis-of-a-monoclonal-antibody
        Sign In To Continue

        To continue reading please sign in or create an account.

        Don't Have An Account?